Almen strips and shot peening intensity: what the arc height really tells you
A single Almen reading is not a shot peening intensity. This guide explains saturation curves, why coverage is a different axis, how media and impact parameters set the ceiling, and which wear and separator faults make the number drift.

Ask a dozen peening shops what intensity they run and you may get a dozen numbers with the same letter attached: "A". That letter is doing a lot of work. A strip of spring steel clamped in a holder and struck on one face is not a fatigue test, not a residual-stress measurement, and not proof that the part in the same basket received an equivalent treatment. It is a repeatable way to put a number on the energy a shot stream delivers. The number only becomes useful when you know how it was obtained.
What the arc height actually measures
An Almen strip is a tightly controlled piece of SAE 1070 spring steel, 76 by 19 mm, peened on one face while held flat. Repeated impacts plastically stretch that face; the stretched layer tries to shorten, the unworked core resists, and the strip curves away from the peened side. A gauge reads the height of that curve — the arc height — in millimetres or thousandths of an inch. It is a proxy for stream energy, not a direct reading of compressive stress inside a gear, spring or blade.
Three standard strip types share the same length and width; only thickness changes. Under SAE J443 guidance, type N is used below 0.10 mm A, type A covers roughly 0.10 to 0.60 mm A, and type C is used above 0.60 mm A. Thickness decides how far a strip bends under the same stream, which is why the type is chosen for the intensity being measured, not for the part being processed. Outside its useful band, a strip bends too little to read reliably or too far to stay linear.
This also means readings should never be converted between strip families. The approximate factors that circulate in shops are estimates presented as measurements, and they rarely survive a customer audit. If the process moves outside the current strip's band, change to the right type and build a fresh curve.
Saturation turns a reading into an intensity
One strip produces one number. It does not produce an intensity. Peening intensity is the arc height at saturation: the point where doubling exposure time adds no more than about ten percent to the arc height. Finding it takes a series of strips peened at increasing times — SAE J443 and J2597 practice calls for at least four points — plotted as arc height against time. Where the curve flattens is the saturation time, and the height at that point is the intensity, always reported with the strip family.
A common audit finding is a process sheet stating a target with no saturation curve behind it. The recorded strip may still have been climbing steeply, or it may have sat in the stream long after useful work stopped. Both produce the same-looking number and very different parts.
Coverage is a separate axis and a separate mistake. The industry convention treats about 98 percent indentation coverage as "full" visual coverage, verified on a coupon of the same material and finish under ten to twenty times magnification, or with fluorescent tracer where geometry hides the surface. A specification for 200 percent coverage means twice the exposure time needed for full coverage; it is a time multiplier, not a surface you can inspect. Pushing far beyond it — roughly the 200 to 300 percent range and upward — tends to roughen the surface and fold metal over without a proportional fatigue benefit. Meanwhile a strip can saturate while a fillet or recess on the actual part remains shadowed. Intensity and coverage must both be specified, and checked at the least accessible feature rather than the easiest one.
Building a setup you can reproduce

Media choice sets the ceiling. Choose the smallest shot that reaches the target intensity: larger particles carry more energy per impact but leave a coarser finish and fewer impacts per square centimetre, and their diameter must still clear the part's smallest inside radius. Cast steel shot to SAE J444 is the economical workhorse; conditioned cut wire to SAE J441 resists breakdown and holds a tighter operating mix; ceramic or stainless media avoid embedded iron on stainless and non-ferrous work. Media hardness should be only slightly above the workpiece. Too soft, and intensity falls; too hard, and particles fracture on impact instead of deforming the surface.
Then lock the rest of the chain: wheel speed or air pressure, nozzle bore and stand-off distance, impingement angle, media flow rate, fixture rotation, and exposure time. Ninety degrees is the most efficient impact angle; glancing angles lose intensity and must be compensated deliberately. Every one of those parameters belongs in the process record, because changing any of them — a new shot size, a different media supplier, a reprogrammed traverse — invalidates the saturation curve.
Exposure time is where cycle time and intensity are most often confused. On a through-feed machine, time in the blast zone is zone length divided by belt or chain speed; in a batch machine it is the programmed dwell. Longer dwell improves coverage and raises arc height only until saturation. If intensity falls short after the curve has flattened, the answer is more impact energy through speed or a suitable media change, not another minute on the conveyor.
Extraction belongs in the same conversation. The air-wash separator removes broken grains and fines before media returns to the wheel, and it needs a full-width falling curtain to work — airflow will find any gap and short-circuit through it. Too little airflow sends fragments back to be broken again, pulling intensity down; too much carries sound shot into the collector. Watch filter differential pressure and sieve the recovered mix weekly. Weighing a shift of collector discharge is a quick check: a loss of a few percent of the circulating charge points to a separator setting or a duct problem, not to poor media quality.
Failure modes that make the number drift
- A single strip instead of a curve — no saturation evidence means the reported intensity cannot be defended, however plausible the number looks.
- Wrong strip family or converted readings — a value estimated from another type hides a real shift in energy and fails audits.
- Media drift — broken or angular grains, an aging mix, or a changed make-up rate lower intensity and raise roughness at the same time.
- Wear in the delivery path — worn nozzle bores, blades, impellers or control cages change velocity and the impact footprint while the machine's speed display stays perfectly correct.
- Fixture and motion drift — datum wear, loose clamps, backlash or a skipped index moves the part out of the qualified stream; a holder placed elsewhere will not see it.
- Air-wash and filter drift — shifted damper settings or a loaded cartridge change the operating mix, and therefore the intensity, without any recipe change on screen.
The routine is short: qualify one saturation curve per setup, keep a coverage coupon, sieve the mix weekly, log parameters alongside every Almen reading, and re-verify after any intervention on the media path. When specifying new equipment, insist on service access to wheels, separators and fixture datums — otherwise these checks become an annual shutdown project.